| 铝镍钴 |
Alnico magnets, composed of primarily
aluminum, nickel, and cobalt, were developed in
the 1940's. This class of magnet remains a
preferred material because of it's excellent
temperature stability, high magnetic flux density,
and resistance to corrosion. Alnico magnets are
manufactured through a casting or sintering
process. The casting process allows for the magnet
to be manufactured into intricate and complex
shapes, which are not possible with other magnetic
materials. |
Typical Magnetic
Performance for Alnico Magnet
|
|
|
Grade |
Br |
Hc |
(BH)max |
Curie Temp |
Temp.Coe |
US standard |
IEC standard |
|
[mT] [Gs] |
[KA/m] [Oe] |
[KJ/m3] [MGOe]
|
[℃] |
[%/℃] |
MMPA Equivalent |
IEC Equivalent
|
|
LN10 |
650 6500 |
42 530 |
10.0 1.20 |
810 |
0.030 |
Alnico 3 |
Alnico 9/3 |
|
LNG11 |
720 7200 |
37 480 |
11.2 1.40 |
810 |
0.030 |
Alnico 1 |
Alnico 8/4 |
|
LNG13 |
700 7000 |
50 620 |
13.0 1.60 |
810 |
0.030 |
Alnico 2 |
Alnico 12/6 |
|
LNGT18 |
580 5800 |
90 1130 |
18.0 |
860 |
0.025 |
[I.Alnico 8] |
Alnico 17/9 |
|
LNG16 |
800 8000 |
53 660 |
16.0 2.00 |
850 |
0.025 |
[Alnico 4] |
/ |
|
LNG34 |
1180 11800 |
44 550 |
35.0 4.30 |
860 |
0.020 |
[Alnico 5C] |
/ |
|
LNG37 |
1180 11800 |
48 600 |
37.0 4.65 |
860 |
0.020 |
Alnico 37/5 |
|
LNG40 |
1220 12200 |
48 600 |
40.0 5.00 |
860 |
0.020 |
Alnico 5 |
/ |
|
LNG44 |
1220 12200 |
52 650 |
44.0 5.50 |
860 |
0.020 |
Alnico 44/5 |
|
LNG52 |
1250 12500 |
55 690 |
52.0 6.50 |
860 |
0.020 |
Alnico 5 DG |
Alnico 52/6 |
|
LNG60 |
1300 13000 |
56 700 |
60.0 7.50 |
860 |
0.020 |
Alnico 5~7 |
/ |
|
LNGT28 |
1050 10500 |
56 700 |
28.0 3.50 |
860 |
0.020 |
Alnico 6 |
Alnico 26/6 |
|
LNGT32 |
800 8000 |
104 1300 |
34.0 4.25 |
860 |
0.025 |
Alnico 8 |
Alnico 38/11 |
|
LNGT38 |
820 8200 |
110 1380 |
38.0 4.75 |
860 |
0.025 |
|
LNGT44 |
880 8800 |
120 1500 |
44.0 5.50 |
860 |
0.025 |
/ |
|
LNGT60 |
900 9000 |
110 1380 |
60.0 7.50 |
860 |
0.025 |
Alnico 60/11 |
|
LNGT72 |
1050 10500 |
112 1410 |
72.0 9.00 |
860 |
0.025 |
Alnico 9 |
/ |
|
LNGT36J |
700 7000 |
140 1750 |
36.0 4.50 |
860 |
0.025 |
Alnico 8 HC |
Alnico 36/15
| |
| 钐钴
|
Samarium
Cobalt (SmCo) magnets, of the Rare Earth class,
have been available since the early 1970's. These
magnets possess very high magnetic properties,
excellent thermal stability, while remaining
resistant to corrosion. These characteristics make
SmCo magnets ideal for applications requiring a
resistance to wide-ranging temperatures and
environments. SmCo magnets are manufactured
by sintering or compression bonding. They are
anisotropic and can only be magnetized in the
direction of orientation. In general, magnetizing
fields of approximately 30 to 45KOe are required
to saturate SmCo magnets. |
|
Typical Magnetic
Performance for Sintered SmCo |
| Grade |
Br |
HcB |
HcJ |
(BH)max |
Curie Temp. |
Temp.Coe |
working T. |
ALLOY
Series |
[mT] [Gs] |
[KA/m] [Oe] |
[KA/m] [Oe] |
[KJ/m3] [MGOe]] |
[℃] |
[%/℃] |
[℃]
|
|
SmCo18 |
800 8000 |
640 8000 |
1430 18000 |
144 18.0 |
750 |
0.04 |
250 |
1:5 |
|
SmCo20 |
850 8500 |
640 8000 |
1590 20000 |
160 20.0 |
750 |
0.04 |
250 |
|
SmCo22 |
900 9000 |
650 8200 |
1430 18000 |
176 22.0 |
750 |
0.04 |
250 |
|
SmCo24 |
980 9800 |
676 8500 |
1430 18000 |
192 24.0 |
800 |
0.04 |
300 |
2:17 |
|
SmCo26L |
1050 10500 |
410 5150 |
432 5430 |
208 26.0 |
800 |
0.04 |
300 |
|
SmCo26 |
1000 10000 |
716 9000 |
1194 15000 |
208 26.0 |
800 |
0.04 |
300 |
|
SmCo26M |
1000 10000 |
716 9000 |
1590 20000 |
208 26.0 |
800 |
0.04 |
300 |
|
SmCo28 |
1030 10300 |
760 9500 |
1430 18000 |
224 28.0 |
800 |
0.04 |
300 |
|
SmCo28H |
1030 10300 |
760 9500 |
1590 20000 |
224 28.0 |
800 |
0.04 |
300 |
|
SmCo30H |
1100 11000 |
480 6000 |
560 7000 |
240 30.0 |
800 |
0.04 |
300
| | |
|
|
|
|